Description for Elantas (Altana) FR-1810
A flexible two-component, low exotherm, flame retardant, long pot life epoxy potting and casting system with excellent handling properties. It is filled with a non abrasive filler to reduce wear on machine metering/dispensing equipment.Brand Cytec Application Type Casting, Potting, Encapsulation 1 Part or 2 Part 2-Part Material Form Liquid Manufacturer Elantas (Altana) Chemistry Epoxy, Non-flammable: Flame-retardant Cure Method Resin/Hardener Cure Temperature (°C) 25, 80 Viscosity (cPs) 8,000, 3,800 Color Black Volume Resistivity (O) 7.1e13 (ohm-cm) Key Specifications Comply with Directive 2011/65/EU, UL (Underwriters Laboratory), ULC (Underwriters Laboratories of Canada), NFPA (National Fire Protection Association): UL 94: UL94 V-0, 4.8 mm -
Technical Data for Elantas (Altana) FR-1810
Overview
-
Application Type
- Casting / Moldmaking - Casting
- Pottant / Encapsulant - Potting, Encapsulation
-
1 Part or 2 Part
- 2-Part
-
Material Form
- Liquid
-
Chemistry
- Non-flammable : Flame Retardant - Flame-retardant
- Epoxy
-
Application Method
- Dispenser - machine metering, dispensing equipment
- Other - Hand-mix Bench Potting / Casting, Meter-mix Bench Potting / Casting, Meter-mix Vacuum Potting / Casting
-
Cure Method
- 2-Part Cure - Resin/Hardener
-
Color
- Black
-
Key Specifications
- RoHS (Restriction of Hazardous Substances) - Comply with Directive 2011/65/EU
- UL (Underwriters Laboratory), ULC (Underwriters Laboratories of Canada), NFPA (National Fire Protection Association) : UL 94 : V0 - UL94 V-0, 4.8 mm
-
Brand
- Cytec
Specifications
Cure Specs
Cure Temperature (°C) 25, 80 Viscosity (cPs) 8,000, 3,800 Test Method Fixture or Handling Strength Time (min) Excellent Set Time (min) 130 Test Method Linear Shrinkage (%) 0.0006 (in/in), 0.06 Test Method Work / Pot Time (min) Long, 80 Test Method Mix Ratio 100:100 (by volume), 100:100 (by weight) Bond Strength
Tensile Strength (psi) 1,325, 1,300 Test Method Conductivity
Dissipation Factor 0.03200, 0.03700, 0.02100, 0.03000, 0.04000, 0.02000 Test Method Filler Non-abrasive filler Dielectric Strength (V/mil) 530 Test Method Dielectric Constant 4.75, 4.39, 3.87, 4.80, 4.40, 3.90 Test Method Thermal Conductivity (W/m°K) 0.70, 0.70 Test Method Surface Resistivity (O) 4.7e15 (Ohm) Test Method Volume Resistivity (O) 7.1e13 (ohm-cm) Test Method Hardness
Shore D Hardness 80 to 85, 80 Test Method Elongation (%) 22, High elongation for reduced stress on components Test Method Flexibility Flexible Business Information
Shelf Life Details CONAPOXY FR-1810 has a shelf life of 18 months from date of manufacture when stored in the original unopened containers at 20C-30C (68F-86F). CONAPOXY FR-1810 Part A and Part B contain filler that may settle during storage. It is recommended that both components be thoroughly mixed before use., Store below 25°C / 77°F in a dry controlled environment out of direct sunlight. This material should be suitable for use stored under these conditions in the original sealed containers for twelve (12) months from the date of shipment. Shelf Life Temperature (°F) 68 to 86, <77 Shelf Life Type From date of manufacture, From the date of shipment Shelf Life (mon) 18, 12 -
-
Best Practices for Elantas (Altana) FR-1810
-
Mixing
Mix and degas individual components thoroughly, prior to use. CONAPOXY® FR-1810 Part A Resin and CONAPOXY® FR-1810 Part B Hardener contain fillers that must be redistributed homogeneously.
Mix FR-1810 Part A and FR-1810 Part B in the ratio specified above until homogeneous. Components may be preheated up to 60°C if reduced viscosity is required. If hand-mixing, degas at >27 in. Hg before use.
-
Curing
Cure 32 - 48 hours at 25°C / 77°F for maximum properties – or – 3 – 4 hours @ 80°C / 176°F
The user is responsible for determining the optimum cure conditions for his application.
-
-
Comparable Materials for Elantas (Altana) FR-1810
Spec Engine® Results
Popular Articles
Testing the effectiveness of surface treatments
Read ArticleInfographic: ENSURING A STRONG BOND - 6 Basic Methods of Surface Preparation
Read ArticleEpoxies in the Aerospace Industry
Read ArticleThe effectiveness of adhesives in the wind power industry
Read ArticleSponsored Articles
Unique Advantages of Contact Adhesives
Read ArticleUsing LOCTITE® 454™ is a Valid Option for Engineers Working with a Wide Variety of Materials
Read ArticleSylgard 184 by DOW is the Top Choice for a Transparent, Silicone Encapsulant. Read Why:
Read ArticleCase Study: Creating reliable, corrosion-free bonds with LORD® 406 acrylic adhesive
Read ArticleFeatured Ads

Linear Shrinkage Test Methods
Linear Shrinkage | Test Method | Temp |
---|---|---|
0.0006 (in/in) | ||
0.06 % | ASTM D2566 | 25°C |
Set Time Test Methods
Set Time | Set Temperature | Test Method |
---|---|---|
130 min | 25°C | Gel Time, 200 gm mass, Mixed |
Viscosity Test Methods
Viscosity | Test Method | Temperature |
---|---|---|
8,000 cPs | Mixed, initial | 25°C |
3,800 cPs | Mixed, initial | 38°C |
Work / Pot Time Test Methods
Work / Pot Time | Test Method | Temperature |
---|---|---|
Long | ||
80 min | To reach 100,000 cps, 200 gm mass, Mixed | 25°C |
Tensile Strength Test Methods
Tensile Strength | Test Temperature | Test Method |
---|---|---|
1,325 psi | ||
1,300 psi | 25°C | ASTM D412 |
Dielectric Constant Test Methods
Dielectric Constant | Temperature | Test Method |
---|---|---|
4.75 | 25°C | @ 100 Hz |
4.39 | 25°C | @ 1 KHz |
3.87 | 25°C | @ 1 MHz |
4.80 | 25°C | ASTM D150, @ 100 Hz |
4.40 | 25°C | ASTM D150, @ 1 kHz |
3.90 | 25°C | ASTM D150, @ 1 MHZ |
Dielectric Strength Test Methods
Dielectric Strength | Temperature | Test Method |
---|---|---|
530 V/mil | 25°C | ASTM D149, 1/16” |
Dissipation Factor Test Methods
Dissipation Factor | Temperature | Test Method |
---|---|---|
0.03200 | 25°C | @ 100 Hz |
0.03700 | 25°C | @ 1 KHz |
0.02100 | 25°C | @ 1 MHz |
0.03000 | 25°C | ASTM D150, @ 100 Hz |
0.04000 | 25°C | ASTM D150, @ 1 kHz |
0.02000 | 25°C | ASTM D150, @ 1 MHZ |
Surface Resistivity Test Methods
Surface Resistivity | Temperature | Test Method |
---|---|---|
4.7e15 (Ohm) | 25°C | ASTM D257 |
Thermal Conductivity Test Methods
Thermal Conductivity | Test Method |
---|---|
0.70 W/m°K | |
0.70 W/m°K | ASTM D5930 |
Volume Resistivity Test Methods
Volume Resistivity | Temp (°C) | Test Method |
---|---|---|
7.1e13 (ohm-cm) | 25°C | ASTM D257 |
Elongation Test Methods
Elongation | Test Method |
---|---|
22 % | ASTM D412, 25°C |
High elongation for reduced stress on components |
Shore D Hardness Test Methods
Shore D Hardness | Shore Hardness Test Method | Hardness Temperature |
---|---|---|
80 to 85 | ||
80 | ASTM D2240 | 25°C |